You are here: Home / Blog / PA66 GF30 Properties: Dry vs Conditioned Datasheet Guide

PA66 GF30 Properties: Dry vs Conditioned Datasheet Guide

Views: 0     Author: Kitty Lee     Publish Time: 2026-11-21      Origin: Site

Inquire

facebook sharing button
twitter sharing button
line sharing button
wechat sharing button
linkedin sharing button
pinterest sharing button
whatsapp sharing button
kakao sharing button
snapchat sharing button
telegram sharing button
sharethis sharing button
PA66 GF30 Properties: Dry vs Conditioned Datasheet Guide

PA66 GF30 is 30% glass-filled nylon 66, the reinforced grade engineers reach for when a part has to carry load at temperature. This guide covers the datasheet values that matter: mechanical properties, heat deflection temperature (HDT), moisture absorption, shrinkage, and molding settings. It also explains the dry-versus-conditioned split that most supplier pages leave out, and compares the material against PA6 GF30, PBT GF30, PPA, and PPS.

If you need a quick answer: choose PA66 GF30 for parts that carry load in heat and humidity or touch coolant; choose PBT GF30 for tight tolerances in humid service; choose PA6 GF30 for cost-sensitive structural parts that stay cool; move to PPA or PPS only when the temperature or moisture demands exceed what PA66 can hold.

Quick decision at a glance

If your part must…

Start with

Why

Carry load at temperature

PA66 GF30

HDT 242–255°C, high dry strength

Hold tight tolerances in humidity

PBT GF30

Near-zero moisture uptake

Stay cheap and keep below ~120°C

PA6 GF30

Easier flow, lower cost

Run hot and wet beyond nylon

PPA GF30 or PPS GF40

Higher HDT, very low moisture

Contents

  1. What 30% Glass Does to Nylon 66

  2. Mechanical Properties: Dry vs Conditioned

  3. Thermal Limits

  4. Density, Moisture Absorption & Shrinkage

  5. PA66 GF30 vs PA6 GF30

  6. PA66 GF30 vs PBT GF30

  7. Higher-Heat Alternatives: PPA and PPS

  8. Injection Molding Parameters

  9. Specifying and Verifying the Grade

  10. Common Failure Modes

  11. Commercial Grades, Variants, and Cost

  12. Long-Term Performance and Environment

  13. Decision Framework

  14. Frequently Asked Questions

Key figures at a glance (typical range across commercial grades, dry at 23°C unless noted)

Property

Typical range

Unit

Test standard

Density

1.36–1.38

g/cm³

ISO 1183

Tensile strength (dry)

170–200

MPa

ISO 527-2

Tensile modulus (dry)

9,500–10,000

MPa

ISO 527-2

Heat deflection temperature, 1.8 MPa

242–255

°C

ISO 75-2/A

Melting point

260–263

°C

ISO 11357-3

Equilibrium moisture absorption, 50% relative humidity (RH)

1.5–2.0

%

ISO 62

Mold shrinkage (flow / transverse)

0.3–0.4 / 0.9–1.2

%

ISO 294-4

Single-grade values below are cited by producer; the ranges span the four grades in the comparison table near the end of this guide. The HDT range covers standard grades only; flame-retardant grades run lower (about 230°C, covered below).

What 30% Glass Does to Nylon 66

The grade code

PA66 is polyamide 66, a semicrystalline nylon made from hexamethylenediamine and adipic acid. "GF30" means the compound carries 30% glass fiber by weight. In practice that is short chopped E-glass dispersed in the polymer, usually with heat stabilizers, impact modifiers, or a flame-retardant package depending on the grade.

Fiber content is the dominant lever on performance. It controls stiffness, strength, heat deflection, and shrinkage. A GF25, GF30, or GF35 grade behaves differently even when the base resin is identical, so treat the number as a hard specification. Different producers also write the same grade differently — PA66-GF30, PA 66 GF30, and nylon 6/6 GF30 all mean the same 30% glass-filled polyamide 66.

Compared with unfilled PA66

Unfilled PA66 has good toughness and chemical resistance, but limited stiffness and dimensional stability. Thirty percent glass changes the picture:

  • Tensile strength more than doubles, from roughly 80 MPa to 170–200 MPa dry.

  • Stiffness roughly triples, from about 3,000 MPa to 9,500–10,000 MPa in tensile modulus.

  • Shrinkage drops and becomes directional: 1.5–2.0% for unfilled PA66, down to 0.3–0.4% along flow but up to 1.2% across it.

The trade-off shows up in processing and design. Glass raises melt viscosity, wears tooling, and cuts elongation at break.

Mechanical Properties: Dry vs Conditioned

This is where most supplier pages mislead. Nylon 66 is hygroscopic. It absorbs moisture from the air until it reaches equilibrium, and as it does, stiffness falls and toughness rises. A mechanical figure for PA66 GF30 means little without the moisture condition attached.

Tensile strength and modulus

In the dry-as-molded state, the grades sit in a tight band. Celanese Zytel 70G30L reports 195 MPa and 9,800 MPa modulus; Domo Technyl A 218 V30 reports 190 MPa and 10,000 MPa; BASF Ultramid A3WG6 reports 185 MPa and 9,500 MPa; Envalior Durethan AKV 30 reports 175 MPa and 10,000 MPa. Conditioned to 50% relative humidity (RH), those values fall to roughly 110–135 MPa and 6,000–7,500 MPa.

The practical question is which number belongs on the drawing. For a part that spends its life in humid air, use the conditioned value. A dry figure is only defensible for a part sealed against moisture, or used for a short-term, one-off check.

chart-tensile-dry-vs-conditioned.png

Figure 1: tensile strength of four commercial PA66 GF30 grades, dry and conditioned. Source: producer technical data sheets.

Flexural strength and modulus

The same split appears in bending. Flexural strength is about 285–290 MPa dry and 185–215 MPa conditioned; flexural modulus runs near 9,000–9,200 MPa dry and 5,800–6,500 MPa conditioned. These are the inputs for a stiffness check on a ribbed housing or a structural bracket.

Impact strength

Impact moves the other way. Nylon toughens as it absorbs water, so Charpy notched impact rises from about 11–13 kJ/m² dry to 14–15 kJ/m² conditioned, with unnotched values around 75–95 kJ/m². Glass reinforcement still costs ductility relative to unfilled nylon: a GF30 part is stiffer and less forgiving of sharp corners.

Thermal Limits: HDT, Melting Point, and Service Temperature

Heat deflection temperature

Heat deflection temperature (HDT) is the thermal figure engineers reach for first, and the one most often misread. HDT records the temperature at which a bar deflects a set amount under a defined load. It says nothing about whether a real part actually fails at that temperature.

At the 1.8 MPa load, the grades measure 242–255°C. At the lighter 0.45 MPa load, they read about 250–260°C. For a load-bearing part, use the 1.8 MPa number.

Melting point and continuous use

The melting point of PA66 is 260–263°C (DSC). That is a processing landmark, and it says little about how hot the part can run. Heat-stabilized PA66 GF30 is generally rated for continuous use around 150°C, with short-term peaks near 220°C depending on the stabilizer package. Confusing HDT or melting point with service temperature is a recurring cause of field failures.

Long-term heat aging

For parts that must survive years at temperature, short-term numbers are not enough. The useful criterion is the temperature at which tensile strength halves after a fixed exposure, such as 20,000 hours under IEC 60216. Heat-stabilized grades hold a temperature index near 140°C over 20,000 hours.

Two different numbers appear here, and they describe different things. The 150°C figure is a general continuous-use rating. The 140°C/20,000 h figure is a specific end-of-life criterion for heat-stabilized (and, in some published data, flame-retardant) grades. Do not compare them directly; request the aging curve for the exact grade.

Density, Moisture Absorption & Shrinkage

Density

PA66 GF30 has a density of 1.36–1.38 g/cm³ (ISO 1183). That feeds part weight and cost calculations, and it is why the material competes with die-cast aluminum for lightweighting: reinforced nylon weighs about half as much as aluminum and needs less machining.

Moisture absorption

Moisture absorption is the best-known weakness of nylon 66 and the reason some engineers strike it from a shortlist. The absorbed water drives both the mechanical changes above and dimensional growth, and the uptake is reversible. The amount depends on the test condition, which is why the two figures are easy to confuse:

  • 24 h immersion in water at 23°C: about 0.7–1.0%

  • Equilibrium at 50% RH: 1.5–2.0%

  • Saturation in water at 23°C: 5.6–6.9%

chart-moisture-uptake.png

Figure 2: water absorption of PA66 GF30 under three test conditions. Source: ISO 62 / similar, producer technical data sheets.

Shrinkage and anisotropy

Mold shrinkage is directional. The grades shrink about 0.3–0.4% along flow and 0.9–1.2% across it (ISO 294-4). A single "0.3–0.7%" figure on a supplier page is not enough to tool a mold. Gate position and wall thickness both shift the split, and mold temperature adds a further shift. A flow-specific value, confirmed by mold-flow simulation, belongs in front of the toolmaker.

Dimensional change in service

Moisture-driven growth continues after molding. A part measured dry will grow slightly as it absorbs water, which can push a tight-tolerance feature out of spec. The fixes are to design to the conditioned dimension or to pre-condition parts before critical measurement, a step many automotive specifications already require.

PA66 GF30 vs PA6 GF30

PA6 GF30 and PA66 GF30 are close relatives and easy to confuse in a selection meeting. Both carry 30% glass and both are strong. The differences are thermal and economic.

PA66 GF30 runs hotter: HDT at 1.8 MPa is 242–255°C against 200–210°C for PA6 GF30, and the melting point is about 260°C versus 220°C. It also retains properties better after moisture absorption and is stronger dry. The trade-off is a higher melt temperature and a narrower processing window, plus a higher resin price.

PA6 GF30 flows more easily and processes cooler, which suits thin-walled or complex parts and keeps the molding bill down. Its lower melting point also shortens cycle time, and impact-modified PA6 grades are typically cheaper per kilogram. That lower cost is the main reason PA6 is the go-to when toughness-for-cost matters more than heat resistance.

Sustained heat, hot coolant, or a demanding load at temperature points to PA66 GF30. A cost-sensitive structural part that stays well below the thermal limit points to PA6 GF30.

PA66 GF30 vs PBT GF30

PA66 GF30 and PBT GF30 compete for connectors, housings, brackets, and sensor bodies. The decision usually comes down to moisture and heat.

PBT GF30 absorbs almost no water, about 0.06–0.08% in 24 hours against 0.7–1.0% for glass-filled nylon. A PBT part holds its dimensions and stiffness in humid service where a nylon part drifts and softens. PBT also molds faster and is electrically stable. Its weaknesses are lower tensile strength (120–140 MPa vs 170–200 MPa), lower heat deflection (200–210°C vs 242–255°C), and poor resistance to hot water, steam, and strong alkalis.

The trade-off runs the other way on heat and coolant. Hydrolysis-stabilized PA66 grades handle hot water and engine glycol that would weaken PBT over time; a general-purpose PA66 grade will still hydrolyze in the same environment, so the stabilizer package is what earns the coolant rating.

Pick PBT GF30 for tight tolerances that must hold in humid conditions, or for precision electrical parts. Pick PA66 GF30 for parts that run hot, carry load at temperature, or touch coolant, provided you specify the hydrolysis-stabilized version.

Higher-Heat Alternatives: PPA and PPS

When PA66 GF30 is not enough, the discussion moves to polyphthalamide (PPA) and polyphenylene sulfide (PPS).

PPA at 30–33% glass (for example, Solvay Amodel A-1133HS, 33% glass) lifts the ceiling: HDT around 285°C at 1.8 MPa (about 297°C at 0.45 MPa), tensile strength around 220–230 MPa dry, and water absorption of only about 0.2% after 24 h immersion. It holds stiffness far better than nylon after conditioning, which is its main selling point. The price is higher, and it needs higher melt temperatures.

PPS GF40 goes further on heat and moisture, with continuous use around 200–220°C and near-zero water uptake (about 0.03%), but it is brittle and costs more than PPA. PPS is the choice for hot, wet, chemically aggressive service where nylon cannot survive.

chart-hdt-comparison.png

Figure 3: HDT at 1.8 MPa for PA66 GF30 and alternatives. Source: producer technical data sheets; PPA and PPS shown for comparison.

In short, PPA buys heat and dimensional stability when PA66 GF30 softens in humid heat, while PPS buys chemical and thermal headroom at a significant cost premium.

Injection Molding Parameters

Processing the grade correctly matters as much as picking it. See the injection molding guide for the full setup. Drying and abrasion dominate the conversation, and high mold temperature is what delivers full crystallinity and stable dimensions.

Drying

Nylon 66 must be dried before molding or it hydrolyzes in the barrel, cutting polymer chains even when the part looks fine. Standard practice is 80°C for about 4 hours in a dry-air dryer, to a residual moisture below 0.2% and ideally near 0.08%. The effect is measurable: molding at 0.3% moisture instead of 0.08% can cut tensile strength by roughly 20% and halve melt viscosity, while leaving silver streaks on the surface (Kunststoff-Profi).

Melt and mold temperature

A melt temperature of 280–300°C is recommended, with 290°C as the usual target. Mold temperature should sit between 80°C and 100°C; pushing toward 120°C improves surface finish and crystallinity but lengthens the cycle. Below about 60°C, crystallinity suffers and glass fibers show at the surface as fiber bloom.

Injection and hold pressure

Injection pressures of 800–1,200 bar (roughly 80–120 MPa) with a hold of 500–800 bar for 5–8 seconds are typical. Weld lines deserve attention: at a knit line, strength can fall to 30–50% of the bulk material, so gates should keep weld lines out of load paths.

Glass-fiber abrasion and tool wear

Glass fiber is abrasive. A barrel and screw running PA66 GF30 should be bimetallic or otherwise hardened, and gates benefit from carbide inserts. Screw life of one to three years is common, depending on screw metallurgy and throughput. This is a real cost of ownership that belongs in the tooling budget.

Specifying and Verifying the Grade

Which standard the numbers come from

Datasheets are not interchangeable. ISO 527 and ASTM D638, or ISO 75 and ASTM D648, use different specimen shapes and methods and can return different values for the same property. A defensible specification states the test standard next to every value, and a datasheet that omits it should be questioned.

Dry vs conditioned: which value to use

Ask the supplier whether the mechanical values are dry or conditioned. For a load-bearing part in a humid environment, the conditioned value is the design input. A datasheet that lists only a high dry tensile strength is showing the best-case number.

Conditioning before measurement

Because nylon drifts as it absorbs water, many specifications require conditioning to 50% RH for 24–168 hours before critical dimensional or mechanical measurement. Skipping it produces results that will not repeat in service.

Red flags in a datasheet

Three omissions justify a follow-up: no test standard, a single shrinkage figure with no flow/transverse split, and no conditioned mechanical values. A supplier that cannot provide those has not characterized the material well enough to support an engineering decision.

Common Failure Modes

Three typical patterns show up in material-selection and after-sales work. None of them appears on a datasheet.

The first is designing to dry data. A bracket specified against the dry tensile strength, then run in a humid plant, comes out softer and slightly larger than the drawing assumed. The part usually still works, but snap-fit forces and the fits against metal inserts drift. Re-running the finite element analysis (FEA) with conditioned values is cheap insurance compared to retooling.

The second is weld-line placement. A housing with two opposing gates puts a knit line straight through a load-bearing boss. The part cracks in test, and the fix is a gate move rather than a stronger material.

The third is shrinkage treated as a single number. A gear blank quoted at 0.5% shrinkage, tooled without a flow/transverse split, ends up out-of-round because the radial and tangential directions shrink differently. This shows up as dimensional scrap, almost always traceable to a datasheet with one shrinkage figure.

Commercial Grades, Variants, and Cost

Main commercial grades

Engineers searching "PA66 GF30 datasheet" are usually looking for a specific grade. The table lists widely specified grades and their published dry values. Values vary by color and lot; confirm against the current technical data sheet (TDS).

Grade

Producer

Tensile strength, dry (MPa)

Tensile modulus, dry (MPa)

HDT 1.8 MPa (°C)

Density (g/cm³)

Ultramid A3WG6

BASF

185

9,500

245

1.37

Zytel 70G30L

Celanese (formerly DuPont)

195

9,800

253

1.37

Technyl A 218 V30

Domo (formerly Solvay)

190

10,000

255

1.36

Durethan AKV 30

Envalior (formerly LANXESS)

175

10,000

242

1.36

Brand ownership has shifted in recent years. Zytel moved to Celanese with DuPont's Mobility & Materials business in 2022, and Durethan moved to Envalior in 2023. Older drawings may still name DuPont or LANXESS; the material is the same, but obtain the current datasheet from the new owner.

Glass content and flame-retardant variants

Glass content can be raised or lowered to suit the part. GF25 lowers stiffness and cost for less demanding parts; GF35 and GF50 push stiffness and heat resistance up, at the cost of higher melt viscosity and more tool wear. Flame-retardant PA66 GF30 grades reach UL94 V0, but the FR package trades away strength and heat: BASF Ultramid A3U42G6 (PA66-GF30 FR) reports about 130 MPa dry tensile strength and an HDT near 230°C.

Other producers

The four grades above are the most widely cited, but they are far from the only options. Other PA66 GF30 sources include Syensqo and Solvay compounds, DSM/Envalior Akulon grades, and Radilon A from RadiciGroup. In China, domestic producers such as Kingfa and Shenma offer lower-cost 30% glass-filled PA66 for local tooling and high-volume parts. Whether these matter depends on your supply base and target market; a North American or European program often specifies a Western brand, while a China-localized part may start with a domestic grade.

Indicative cost

People searching "PA66 GF30 price" usually want a number to put into a bill of materials. As a planning figure, injection-molding grades of 30% glass-filled PA66 traded around US$3.50–5.50/kg at 1–5 tonne annual volume in 2025, with the glass fill itself adding roughly $0.80–1.20/kg over unfilled resin (engineering plastic price guide, 2025). Domestic Chinese compounds sit in a similar or lower band. These are indicative ranges that move with region, volume, oil prices, and resin market conditions, so request a quote for the specific grade rather than relying on a published number.

Long-Term Performance and Environment

Electrical performance (CTI)

For electrical parts, the comparative tracking index (CTI) matters more than tensile strength. Zytel 70G30L carries a published CTI of 600 V; Durethan AKV 30 measures 475 V; Technyl A 218 V30 measures 400 V; Ultramid A3WG6 measures about 450 V. CTI is not directly comparable across grades unless the test conditions match: IEC 60112 allows different test solutions (solution A is the more demanding and returns lower voltages) and specimen thicknesses, so only compare values tested the same way.

Creep, fatigue, and thermal expansion

Creep and fatigue are what make the grade a long-term metal replacement, and they need specific values rather than generalities. The BASF Ultramid A3WG6 HRX datasheet lists a tensile creep modulus of 4,800 MPa after 1,000 h at 0.5% strain and 23°C, conditioned (ISO 899-1); the standard A3WG6 lists 5,300 MPa under the same conditions, so pull the curve for your exact grade. For fatigue, supplier S-N curves typically show a fatigue strength in the region of 30–40% of the dry tensile strength at 10⁷ cycles, though this varies enough by grade and stress state that a design should not rely on the rule of thumb.

The coefficient of linear thermal expansion (CLTE) is anisotropic, about 28–30 × 10⁻⁶/K along flow and 90–95 × 10⁻⁶/K across it (Zytel 70G30L datasheet), which matters when a plastic part must match a metal insert.

Chemical resistance, weathering, and color

Nylon 66 resists oils, greases, fuels, and aliphatic hydrocarbons, and is attacked by strong acids, oxidizing agents, and some phenols. Hot water and steam cause hydrolysis unless the grade is stabilized. Outdoors, nylon chalks and embrittles under UV unless UV-stabilized, and carbon-black grades weather noticeably better than natural grades. Color also shifts other properties slightly: black grades can show marginally lower moisture uptake than natural, so confirm the TDS for the color you will actually mold.

Regrind and recycled content

Regrind shortens glass fibers on reprocessing, trimming tensile and impact a few percent per pass. Typical supplier guidance caps regrind at 20–30% for structural parts, with property validation per run and sign-off from the supplier.

Decision Framework

Requirement

Best fit

Reason

High heat and load at temperature

PA66 GF30

HDT 242–255°C, high dry strength

Hot water, glycol, coolant contact

PA66 GF30, hydrolysis-stabilized

Stabilized nylon survives coolant; PBT hydrolyzes in hot glycol over time

Cost-sensitive structural part, no thermal limit

PA6 GF30

Easier flow, lower cost, adequate strength

Tight tolerance in humid service

PBT GF30

Near-zero moisture uptake, stable dimensions

Precision electrical part, fast cycles

PBT GF30

Dimensional and electrical stability

Impact-prone clips and fasteners

PA6 GF30

Lower cost for adequate toughness

Hot, humid service beyond nylon's reach

PPA GF30

Higher HDT, low moisture, keeps stiffness

Hot, wet, chemically aggressive service

PPS GF40

Continuous use to ~220°C, near-zero uptake

PA66 GF30 vs PA6 GF30 vs PBT GF30 (typical 30% glass values)

Property

PA66 GF30

PA6 GF30

PBT GF30

Density (g/cm³)

1.36–1.38

1.35–1.37

1.52–1.54

Tensile strength, dry (MPa)

170–200

150–185

120–140

HDT at 1.8 MPa (°C)

242–255

200–210

200–210

Water absorption, 24 h immersion (%)

0.7–1.0

0.9–1.2

0.06–0.08

Equilibrium moisture, 50% RH (%)

1.5–2.0

2.0–2.8

~0.1

Melting point (°C)

260–263

~220

~225

Sources: PA66 GF30 figures from BASF, Celanese, Domo, and Envalior technical data sheets. PA6 GF30 and PBT GF30 figures are typical ranges compiled from comparative sources (ResinBridge, Beskamold); confirm these against the specific grade's original datasheet, as the density and moisture values in particular vary by producer. "24 h immersion" and "Equilibrium 50% RH" are different tests and should not be read as the same figure.

Frequently Asked Questions

What is the tensile strength of PA66 GF30?

Dry as molded, commercial grades sit between 170 and 200 MPa: Ultramid A3WG6 185 MPa, Zytel 70G30L 195 MPa, Technyl A 218 V30 190 MPa, Durethan AKV 30 175 MPa. After conditioning at 50% RH, tensile strength falls to roughly 110–135 MPa.

What is the density of PA66 GF30?

Density is 1.36–1.38 g/cm³ (ISO 1183), between unfilled PA66 at about 1.14 g/cm³ and PBT GF30 at about 1.52 g/cm³.

What is the heat deflection temperature of PA66 GF30?

HDT at 1.8 MPa is 242–255°C and at 0.45 MPa about 250–260°C. HDT is a test value, not an operating limit; heat-stabilized grades are typically rated for continuous use around 150°C.

How much moisture does glass-filled nylon 66 absorb?

It depends on the test. About 0.7–1.0% after 24 h immersion, 1.5–2.0% at equilibrium in 50% RH, and 5.6–6.9% at saturation in water at 23°C. The absorbed water softens and swells the material.

How does PA66 GF30 compare with PA6 GF30?

PA66 GF30 has higher heat deflection (242–255°C vs 200–210°C), a higher melting point, and better property retention after moisture absorption, but costs more and needs a higher melt temperature. PA6 GF30 flows more easily and suits cost-sensitive parts that stay cool.

How does PA66 GF30 compare with PBT GF30?

PA66 GF30 is stronger (170–200 MPa vs 120–140 MPa) and more heat-resistant, but absorbs far more moisture (0.7–1.0% vs 0.06–0.08% in 24 h). PBT GF30 holds tighter tolerances in humid service; PA66 GF30 wins on heat, toughness, and coolant contact when hydrolysis-stabilized.

How does PA66 GF30 compare with PPA?

PPA GF30/GF33 has a higher HDT (about 285°C at 1.8 MPa vs 242–255°C), higher dry tensile strength, and much lower moisture absorption (about 0.2% after 24 h). It costs more and needs higher melt temperatures. Choose PPA when humid heat pushes nylon beyond its limit; choose PA66 GF30 when cost matters and the thermal demands are within nylon's range.

What temperature can PA66 GF30 withstand?

Continuous use is typically around 150°C for heat-stabilized grades, with short-term peaks near 220°C. The 242–255°C HDT is a deflection test value, not an operating limit.

Does PA66 GF30 need to be dried before molding?

Yes. Dry at 80°C for about 4 hours to a residual moisture below 0.2% (ideally 0.08%). Undried resin hydrolyzes in the barrel, cutting tensile strength and leaving surface defects.

How much does PA66 GF30 cost?

As a planning figure, injection-molding grades traded around US$3.50–5.50/kg at 1–5 tonne annual volume in 2025. The price moves with region, volume, and resin markets, so request a quote for the specific grade.

How much regrind can be used with PA66 GF30?

Typical supplier guidance caps regrind at 20–30% for structural parts, with property validation per run. Regrind shortens glass fibers and trims tensile and impact a few percent per pass.

Does PA66 GF30 need UV stabilization?

Only for outdoor exposure. Unstabilized nylon chalks and embrittles under UV; UV-stabilized or carbon-black grades weather noticeably better. Indoor parts generally do not need it.

Dongguan Quanhao Plastic Mold Co., Ltd. has been focus on plastic injection mold and Plastic parts ever since its fundation.
Leave a Message
Contact Us

Product Category

Services

Quick Links

Copyright © 2024 Dongguan Quanhao Plastic Mold Co., Ltd.  All rights reserved.  Sitemap I  Privacy Policy